I've complete my assg.
I found out that to produce the PS take-away hinged box,the raw materials are:
PS pellet (yield by suspension polymerization).....94-96%
blowing agent (g) (CFC, CO2, 1,1-difluoroethane, pentane)....4-6%
nucleating agent .....<0.25%
The nucleating agent would be put into the single screw extruder@ 150-205 C, 1000-2000psi.
Blowing agent would then be putting in using high pressure.
The homogenized PS would start foaming aft exit the die.
And then the PS foam would be pull towards cooling mandrel, rolll-up and left for >24hr for aging.
The extruded sheet would be used to thermo form into the desired product.
The PS box is white in color because in extruder, when the polymer is compressed and because the change of phases from clear amorphous stage to semi-crystallized stage.